DAITOSOL

Transcription

DAITOSOL
DAITOSOL
www.daitokasei.com
No.10
Revised: 12 May, 2015
DAITO KASEI KOGYO Co.,LTD.
DAITOSOL
I. What is DAITOSOL?
Alkyl acrylate copolymer emulsion is the film former, which is widely
used in cosmetic field.
DAITOSOL have been used for over 35 years.
II. Advantage of DAITOSOL
DAITOSOL give the following unique properties for cosmetic products:
(1) Flexible and Strong Film
(2) Long Lasting Glossy Thin Film
(3) Water Resistant Film
DAITOSOL have been used over 35 years because of its high safety.
Recently, DAITOSOL are used for not only mascara and eye liner, but
also for the skin care and body care product for its very unique and
flexible film.
III. Low Level of Residual Monomer of DAITOSOL
For more and more concern about residual monomer for alkyl acrylate
copolymer, we guarantee the following level for our DAITOSOL.
Spec Value
DAITOSOL 5000AD
DAITOSOL 5000SJ
Residual Monomer
Less than 40 ppm
(As Ethyl acrylate)
Less than 80 ppm
(As n-Butyl acrylate)
Ref. JCIC Spec.
Less than 1.5%
Less than 1.5%
-1-
DAITOSOL
Product Name
INCI Name
DAITOSOL 5000AD
DAITOSOL 5000SJ
DAITOSOL 4000SJT
DAITOSOL 5000STY
Acrylates Copolymer
Acrylates/Ethylhexyl
Acrylate Copolymer
Acrylates/Ethylhexyl
Acrylate Copolymer
Styrene/Acrylates
Copolymer
Appearance
Milky White emulsion
5000AD
5000SJ
4000SJT
5000STY
5500GM
5000SJ
4000SJT
5000PO
Film
Appearance
T
Transparent,
t Glossy
Gl
Tackiness
5000GM > 5000AD > 5000STY = 5000SJ = 4000SJT > 3000VP3 > 3000SLPN-PE1 = 5000PO
Particle size
(nm)
140
130
60
125
Viscosity
(mPa・s)
50-150
50-200
50
600
pH
5.5 - 7.5
2.0 - 5.0
2.0 - 5.0
7.0 – 8.0
Solid content
(%)
50
50
40
50
Tg (℃)
-14
-13
-13
7
Sodium
dehydroacetate
None
(Low pH)
None
(Low pH)
Sodium
dehydroacetate
Preservative
Property
Fl ibl & S
Soft
ft Fil
Film
- Flexible
G d Fl
Flexibility
ibilit
- Good
G d Fl
Flexibility
ibilit
- Good
- Excellent Adhesion
- Good Balance of
- Good Balance of
- Can incorporate
Water Resistancy
Water Resistancy and
with fiber and beads
and Removability
Removability
as fixer
- Preservative Free
- Preservative Free
-2-
- Super
p Long
g Lasting
g
- Excellent Water
Resistancy
- Excellent adhesion to
skin
- Rub-off Resistance
DAITOSOL
Product
Name
DAITOSOL 5500GM
DAITOSOL
3000SLPN-PE1
DAITOSOL
3000VP3
DAITOSOL 5000PO
INCI Name
Acrylates/Ethylhexyl
Acrylate Copolymer
Acrylates Copolymer
Acrylates Copolymer
Acrylates/Ethylhexyl
Acrylate Copolymer
Appearance
Milky White emulsion
White liquid
Transparent
Milky White emulsion
3000SLPN-PE1
3000VP3
Transparency of appearance
3000VP3 > 3000SLPN-PE1 > 4000SJT > 5000PO
> 5000SJ = 5000STY = 5500GM > 5000AD
Film
Appearance
Transparent, Glossy
Tackiness
5000GM > 5000AD > 5000STY = 5000SJ = 4000SJT > 3000VP3 > 3000SLPN-PE1 = 5000PO
Particle size
(nm)
160
50
20
100
Viscosity
(mPa・s)
3000
30
15,000
1,000
7.0 - 8.5
7.0 - 9.0
7.0 - 9.0
6.5-8.5
Solid content
(%)
55
30
30
50
Tg (℃)
-67
37
25
10
Sodium
dehydroacetate
Phenoxyethanol
Phenoxyethanol
Sodium
dehydroacetate
pH
Preservative
- Superior Tackiness
- Good Adhesion to
Property
- Hard Film
skin
- High Tg, Hard Film
- High Viscosity
- Glue for artificial
- Good Transparency
- Excellent
eyelash
- No Tackiness
Transparency
- Glue for double eye
- Less Tackiness
lid
-3-
- Good Balance of
Water Resistancy
and Removability
- For Peel Off
Aqueous Manicure
- Tack Free
DAITOSOL
 DAITOSOL Map
Tg(℃)
Hard
3000SLPN PE1
3000SLPN-PE1
3000VP3
5000PO
O
5000STY
0℃
4000SJT
5000SJ
Soft
5000AD
5500GM
High
Low
Water Resistancy
 Mechanical Property
Modulus (Mpa)
1.80
1.50
5000AD
1.20
5000SJ
0.90
4000SJT
5000STY
0.60
0.30
0.00
0
500
1000
1500
2000
2500
Elongation (%)
-4-
3000
3500
4000
Suggested Formula
1. As Film former
2. As Glue
BODY GLIMMER
For False Eye Lash
MASCARA&EYE LINER
POINT MAKE-UP
FOUNDATION &
SUN SCREEN
For Double Eye Lid
DAITOSOL
3. For Peeling
PEELING MOUSSE
4. For Lifting
LIFTING GEL
PEELING CREAM
Tightening Effect
-5-
1. As Film former
Long Lash & Volume-up Mascara
No. DM/014
<Phase>
<%>
<Ingredient>
A
A
A
A
A
A
A
CARNAUBA
BEESWAX
STEARIC ACID
GLYCERYL STEARATE SE
5.50
9.00
2.00
2.00
2.00
2.00
5.00
B
B
B
B
B
WD-IOB50
DE-IONIZED WATER
MAKILENE GC
AMINOMETHYL PROPANEDIOL
PRESERVATIVE
C
DAITOSOL 5000STY
PROPYLENE GLYCOL STEARATE
POLYISOBUTENE
DIMETHICONE
<Trade Name>
<Supplier>
LUNAC S-98
RHEODOL MS165V
HOMOTEX PS-200
Kao Chemicals
Kao Chemicals
Kao Chemicals
KF-96L-2CS
Shin Etsu
20.00
19.70
2.00
0 50
0.50
0.30
TOTAL :
30.00
100.00
TOTAL :
97.00
3.00
100.00
(FINAL COMPOUND)
MASCARA BASE
NFCB-17D-6R
DAITO KASEI
DKE
DAITO KASEI
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Heat the mixture of Phase A and Phase B to 80C separately.
+28.7 %
longer
2. Adjust loss of water and dimethicone evaporated during heating.
3. Add Phase A into Phase B, and keep stirring until the mixture is homogeneous.
4. Add Phase C under stirring below 50C.
5. M ix well fiber in mascaea base.
Eye Lash Model
Length: 9.92mm
Length: 7.71mm
Volume: 17.60mm2
Volume: 10.57mm2
+66.5 %
volume-up
Super Long Lasting Eye Liner
No. DE/001
<Phase>
A
A
A
A
<%>
8.50
0.20
1.00
0.30
<Ingredient>
DE-IONIZED WATER
XANTHAN GUM
MAKILENE GC
PRESERVATIVE
B
WD CB2
WD-CB2
C
C
DAITOSOL 3000SLPN
DAITOSOL 3000VP3
TOTAL :
<Trade Name>
<Supplier>
KELTROL CG-T
SANSHO
DKE
20 00
20.00
DAITO KASEI
20.00
50.00
100.00
DAITO KASEI
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Prepare Phase A.
2. Add Phase B, and Phase C into Phase A under stiring.
Applying
running water
-6-
Rubbing:
10 times
Rubbing:
30 times
Volumizing Separate Mascara
No. DM/015
<Phase>
<%>
<Ingredient>
A
A
A
A
A
A
A
POLYISOBUTENE
DIMETHICONE
B
B
B
B
B
B
WD-IOB50
DE-IONIZED WATER
MAKILENE GC
MAKIMOUSSE 12
AMINOMETHYL PROPANEDIOL
PRESERVATIVE
C
DAITOSOL 5000STY
5.50
9.00
2.00
2.00
2.00
2.00
5.00
CARNAUBA
BEESWAX
STEARIC ACID
GLYCERYL STEARATE SE
PROPYLENE GLYCOL STEARATE
<Trade Name>
<Supplier>
LUNAC S-98
RHEODOL MS165V
HOMOTEX PS-200
Kao Chemicals
Kao Chemicals
Kao Chemicals
KF-96L-2CS
Shin Etsu
20.00
19.60
2.00
0.10
0.50
0 30
0.30
DAITO KASEI
30.00
100.00
DAITO KASEI
TOTAL :
TOTAL :
97.00
3.00
100.00
(FINAL COMPOUND)
MASCARA BASE
CELLULOBEADS D-10(CB2-15)
DKE
DAITO KASEI
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Heat the mixture of Phase A and Phase B to 80C separately.
2. Adjust loss of water and dimethicone(2cs) evaporated during heating.
+18.0 %
longer
3. Add Phase A into Phase B, and keep stirring until the mixture is homogeneous.
4. Add Phase C under stirring below 50C.
5. M ix well CELLULOBEADS in mascaea base.
Eye Lash Model
Length: 9.10mm
Length: 7.71mm
Volume: 18.13mm2
2
V l
Volume:
10.57mm
10 57
+71.5 %
volume-up
Pearly Eye Liner
No. DE-0032-WDFB40
DE 0032 WDFB40
<Phase> <Ingredient>
A
DE-IONIZED WATER
A
MAKILENE GC
A
XANTHAN GUM
A
HECTORITE
A
PRESERVATIVE
Blue
<%>
51.10
1.00
0.70
0.70
0.30
Light Blue
<%>
47.50
1.00
0.70
0.70
0.30
Green Violet
<%>
<%>
51.80
56.60
1.00
1.00
0.70
0.70
0.70
0.70
0.30
0.30
<Trade Name>
<Supplier>
KELTROLCG-T
LAPONITE XLS
DKE
SANSHO
ROCKWOOD
B
B
B
B
WD-FB40
WD-Ti50
WD-IOY50
WD-IOR50
12.00
4.20
-
10.00
9.80
-
3.60
2.00
3.90
-
2.60
1.40
0.70
DAITO KASEI
DAITO KASEI
DAITO KASEI
DAITO KASEI
C
C
C
DK PEARL-GFIF WHITE
DK PEARL GOLD
DK PEARL BORDEAUX
10.00
-
10.00
-
16.00
-
16.00
DAITO KASEI
DAITO KASEI
DAITO KASEI
D
DAITOSOL 5000STY
20.00
TOTAL : 100.00
20.00
100.00
20.00
100.00
20.00
100.00
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Disperse Xanthan gum and Hectorite in butylene glycol and preservative.
2. Add water, heat to 40-50C, and disperse well.
3. Add Phase B into Phase A, and keep stirring until the mixture is homogeneous.
4. Add Phase C into Phase A+B, and keep stirring until the mixture is homogeneous.
5. Add Phase D under stirring.
-7-
Body Glimmer Gel
No. DO-0065-SJ
<Phase>
A
A
A
<Ingredient>
DE-IONIZED WATER
MAKILENE GC
MAKIMOUSSE 12
B
DAITOSOL 5000SJ
C
ETHANOL
D
D
D
DK PEARL SILVER2
DK PEARL BRONZE
DK PEARL GOLD
<%>
61.20
5.00
1.00
<Trade Name>
<Supplier>
DKE
DAITO KASEI
5.00
DAITO KASEI
25.00
TOTAL :
1.50
0.80
0.50
100.00
DAITO KASEI
DAITO KASEI
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Di
1
Disperse MAKIMOUSSE 12 iin MAKILENE GC
GC, and
d add
dd water
t tto prepare gel.
l
2. Add Phase B and C one after another.
3. Add Phase D and keep stirring until the mixture is homogeneous.
Mousse Jelly Eye Shadow
No. DO/015
<Phase>
A
A
A
A
<Ingredient>
DE-IONIZED WATER
MAKILENE GC
PRESERVATIVE
MAKIMOUSSE 25
B
B
B
B
B
B
OTS-2 TALC JA-46R
OTS-2 DK PEARL VIOLET
OTS-2 DK PEARL-SY COPPER
OTS 2 DK PEARL
OTS-2
PEARL-SY
SY GOLD
OTS-2 DK PEARL-GFIF WHITE
CELLULOBEADS D-10
C
DAITOSOL 4000SJT
VIOLET COPPER GOLD
<%>
<%>
<%>
<Trade Name> <Supplier>
73.70
5.00
0.30
1.00
73.70
5.00
0.30
1.00
73.70
5.00
0.30
1.00
4.00
4.00
4.00
3.00
4.00
4.00
4.00
3.00
4.00
4 00
4.00
4.00
3.00
DAITO KASEI
DAITO KASEI
DAITO KASEI
DAITO KASEI
DAITO KASEI
DAITO KASEI
5.00
5.00
5.00
TOTAL : 100.00 100.00 100.00
DAITO KASEI
DKE
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Disperse MAKIMOUSSE 25 in MAKILENE GC and preservative, and add water to prepare gel.
2. Add Phase B into Phase A under stirring.
3. Add phase C into the mixture of phase A+B, and keep stirring until the mixture is homogeneous.
Soufflé Touch Blush
No. DO/018
<Phase>
A
A
A
A
<Ingredient>
DE-IONIZED WATER
MAKILENE GC
PRESERVATIVE
MAKIMOUSSE 12
B
B
B
B
B
B
B
MST-1 TiO2 R250
MST-1 YELLOW No.602P
MST-1 RED No.211P
MST-1 BLACK No.710P
SI-2 D&C RED No.30
MST-3 DK PEARL-IF RED
MST-3 DK PEARL SILVER2
C
DAITOSOL 4000SJT
<%>
<Trade Name> <Supplier>
83.95
5.00
0.30
0.70
DKE
DAITO KASEI
DAITO
DAITO
DAITO
DAITO
DAITO
DAITO
DAITO
0.50
0.15
0.20
0.10
0.10
3.00
1.00
KASEI
KASEI
KASEI
KASEI
KASEI
KASEI
KASEI
DAITO KASEI
5.00
TOTAL : 100.00
<MANUFACTURING PROCEDURE>
1. Disperse MAKIMOUSSE 12 in MAKILENE GC and preservative, and add water to prepare gel.
2. Mix well pigments (Phase B) to obtain a shade, and add Phase B into Phase A under stirring.
3. Add phase C into the mixture of phase A+B, and keep stirring until the mixture is homogeneous.
-8-
Aqueous Manicure
No. DO/037
Red
<Phase> <Ingredient>
(MANICURE BASE)
A
DAITOSOL 3000SLPN
3000SLPN-PE1
PE1
B
B
B
B
B
B
B
Black
<%>
Blue
<%>
Pearl
<%>
Beige
<%>
<%> <Trade Name>
93 00
93.00
93 00
93.00
98 50
98.50
86 10
86.10
7.00
100 00
100.00
1.50
100 00
100.00
11.00
1.00
0.30
0.30
1.00
0.30
100 00
100.00
11.00
1.00
0.30 Laponite XLS
0.30 KELTROL CG-T
1.00 LUCENTITE SWN
0.30
100 00
100.00
DKE
ROCKWOOD
SANSHO
Co-op Chamiecal
TOTAL:
7.00
100 00
100.00
93.00
7.00
100.00
95.00
5.00
100.00
97.50
2 50
2.50
100.00
97.50
0.06
0.22
0.42
1 80
1.80
100.00
DAITO
DAITO
DAITO
DAITO
DAITO
DAITO
TOTAL :
90.00
10.00
100.00
10% ARGININE solution
DE-IONIZED WATER
MAKILENE GC
HECTORITE
XANTHAN GUM
SODIUM M AGNESIUM SILICATE
PRESERVATIVE
(FINAL COMPOUND)
MANICURE BASE
WD-R7-15(BP)
WD-CB2
WD-FB40
WD-IOY50
WD-IOR50
DK PEARL
PEARL-SY
SY SILVER
86 10
86.10
<Supplier>
DAITO KASEI
KASEI
KASEI
KASEI
KASEI
KASEI
KASEI
Aqueous Manicure
No. DO/049
Red
<Phase> <Ingredient>
(MANICURE BASE)
A
DAITOSOL 3000SLPN-PE1
B
B
B
B
B
B
B
<%>
Blue
<%>
Green
<%>
Yellow
<%>
Violet
<%> <Trade Name>
95.00
95.00
95.00
86.10
5.00
100.00
5.00
100.00
11.00
1.00
0.30
0.30
1.00
0 30
0.30
100.00
5.00
Laponite XLS
KELTROL CG-T
LUCENTITE SWN
100.00
DKE
ROCKWOOD
SANSHO
Co-op Chamiecal
TOTAL:
5.00
100.00
96.05
3.95
100.00
96.87
3.13
100.00
96.74
3.26
100.00
96.18
2.34
1.48
100.00
DAITO
DAITO
DAITO
DAITO
TOTAL :
96.25
3.75
100.00
10% ARGININE solution
DE-IONIZED WATER
MAKILENE GC
HECTORITE
XANTHAN GUM
SODIUM M AGNESIUM SILICATE
PRESERVATIVE
(FINAL COMPOUND)
MANICURE BASE
MAKICOLOR WD RED
MAKICOLOR WD BLUE
MAKICOLOR WD GREEN
MAKICOLOR WD YELLOW
95.00
<Supplier>
<MANUFACTURING PROCEDURE>
1. Preparation of M ancure Base Red, Blue,Green, Violet color,
*Red, Blue, Green, Violet* Add 10% ARGININE solution into DAITOSOL 3000SLPN under simple mixing.
*Yellow* Add DAITOSOL 3000SLPN into Phase B littele by littele, and keep stirring untile the mixture is homogeneous.
2. Add WD series into M ANICURE BASE, and keep stirring untile the mixture is homogeneous.
-9-
DAITO KASEI
KASEI
KASEI
KASEI
KASEI
Aqueous Manicure -Soap WashableNo. DO/051
Violet
<Phase> <Ingredient>
(MANICURE BASE)
DAITOSOL 3000VP3
A
B
B
B
<%> <Trade Name>
DE-IONIZED WATER
MAKICOLOR WD RED
MAKICOLOR WD BLUE
TOTAL :
<Supplier>
86.18
DAITO KASEI
10.00
2.34
1.48
100.00
DAITO KASEI
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Prepare Phase A and Phase B.
2. Add Phase B into Phase A and keep stirring at 500rpm for 1 minutes.
Peel Off Aqueous Manicure
No. DO/059
<Phase>
A
A
A
A
A
<Ingredient>
DE-IONIZED WATER
MAKILENE GC
HECTORITE
XANTHAN GUM
PRESERVATIVE
<%> <Trade Name>
11.00
1.00
0.25 Laponite XLS
0.25 KELTROL CG-SFT
0.30
B
B
DAITOSOL 5000PO
ACETYL TRIBUTYL CITRATE
82.20
2.50 CITROFLEX A-4
C
DK PEARL-SY SILVER
2.50
TOTAL : 100.00
<Supplier>
DKE
ROCKWOOD
SANSHO
DAITO KASEI
MORIMURA BROS.,INC.
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Prepare Phase A,
disperse Xanthan gum & laponite XLS in M AKILENE GC and preservative, and add water to prepare gel.
2. Prepare phase B (Add ACETYL TRIBUTYL CITRATE to DAITOSOL 5000PO under stirring).
3 Add Phase B into Phase A
3.
A, and keep stirring until the mixture is homogeneous
homogeneous.
4. Add Phase C into Phase A+B, and keep stirring until the mixture is homogeneous.
- 10 -
Aqueous Wet Effect Lipgloss
No. DLP/021
<Phase>
A
A
A
A
A
A
A
<Ingredient>
OCTYLDODECANOL
MAKIGREEN GF
DK-PGT PASTE R7
DK-PGT PASTE Y5L
DK-PGT PASTE IOR
OTS-2 DK PEARL-SY SILVER
OTS-2 DK PEARL-GFIF WHITE
B
B
B
DE-IONIZED WATER
DAITOSOL 3000VP3
PRESERVATIVE
C
ALCOHOL
Beige
<%>
30.20
11 25
11.25
0.04
0.36
0.45
1.80
5.40
Red
<%>
35.00
13 00
13.00
1.50
-
5.20
44.00
0.30
5.20
44.00
0.30
<Trade Name>
KALCOL 200GD
<Supplier>
Kao
DKE
DAITO KASEI
DAITO KASEI
DAITO KASEI
DAITO KASEI
DAITO KASEI
DAITO KASEI
1.00
1.00
TOTAL: 100.00 100.00
<MANUFACTURING PROCEDURE>
After 30 Minutes
1. Heat Phase A until 80C, mix well, and cool to room temperature.
2. Add Phase B to Phase A under stirring.
3. Add Phase C into Phase A+B, and mix well.
- 11 -
Long Lasting O/W Liquid Foundation
No. DL/045
<Phase>
A
A
A
A
<%>
<Ingredient>
STEARIC ACID
GLYCERYL STEARATE SE
CETYL ALCOHOL
MINERAL OIL
2.50
1.80
0.50
9.90
B
B
B
B
B
ASI TiO2 CR-50
ASI YELLOW LL-100P
ASI RED R-516P
ASI BLACK BL-100P
CELLULOBEADS D-10
8.50
1.00
0.30
0.20
3.00
C
C
C
C
C
DE-IONIZED WATER
MAKILENE GC
XANTHAN GUM
TRIETHANOLAMINE (90%)
PRESERVATIVE
D
DAITOSOL 5000STY
51.60
9.00
0.20
1.20
0.30
TOTAL :
<Trade Name>
<Supplier>
Kao Chemicals
LUNAC S-98
RHEODOL MS165V Kao Chemicals
DAITO
DAITO
DAITO
DAITO
DAITO
KELTROL CG-T
KASEI
KASEI
KASEI
KASEI
KASEI
DKE
SANSHO
DAITO KASEI
10.00
100.00
DL/045 (STY 10%)
<MANUFACTURING PROCEDURE>
BLANK
1. Mix well pigments (phase B) to obtain a shade.
2. Add Phase B into Phase A Under stirring.
3. Prepare Phase C to prepare gel.
4. Heat the mixture of Phase A and Phase C to 80C degree separately.
5. Adjust loss of water evaporated during heating.
6. Add Phase A+B into Phase C , and keep stirring until the mixture is homogeneous.
7. Add Phase D below 40C degree, and mix well.
30 Minutes Later
Stretch Sun Screen
No. DS/002
<Phase>
A
A
A
A
DS/002 BLANK
<%>
<%>
<Ingredient>
PHENYLTRIMETHICONE
TRIDECYL ISONONANOATE
CELLULOBEADS D-10
DIMEHICONE/VINYL DIMETHICONE
CROSSPOLYMER (AND) DIMETHICONE
1.00
3.00
3.00
1.00
1.00
3.00
3.00
1.00
A
A
A
Daitopersion Zn-50
Daitopersion Ti-30
CYCLOMETHICONE
30.00
20.00
5.00
30.00
20.00
5.00
B
B
B
B
B
DE-IONIZED WATER
1,3-BUTYLENE GLYCOL
SODIUM CHLORIDE
PRESERVATIVE
DISODIUM EDTA
19.65
6.00
1.00
0.30
0.05
29.65
6.00
1.00
0.30
0.05
C
DAITOSOL 5000SJ
10.00
100.00
100.00
TOTAL :
<Trade Name>
<Supplier>
KF-56
SALACOS 913
KSG-16
Shin Etsu
Nisshin Oillio
DAITO KASEI
Shin Etsu
KF-995
DAITO KASEI
DAITO KASEI
Shin Etsu
PHENONIP
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Prepare Phase A and Phase B separately.
2. Add Phase B to Phase A and keep stirring until the mixture is homogeneous.
3. Add phase C, and keep stirring until the mixture is homogeneous.
Flexibility of Sun Screen
Applied on the artificial skin (0.08g/40cm2),
dried for 1 hour,
stretched the artificial skin,
and checked the appearance.
DS/002 (+5000SJ 10%)
- 12 -
Blank
2. As Glue
Eyelash Glue
No. DE-0024-GM
<Phase>
A
<Ingredient>
DAITOSOL 5500GM
<%>
<Trade Name>
100.00
TOTAL : 100.00
<Supplier>
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Put Phase A into a suitable container.
Eyelash Glue (Black)
No. DE-0025-GM
<Phase>
A
A
<%>
<Ingredient>
DAITOSOL 5500GM
WD-CB2
TOTAL :
<Trade Name>
90.00
10.00
100.00
<Supplier>
DAITO KASEI
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Mix well Phase A and put into a suitable container.
Eyelash Glue Gel
No. DE-0026-GM
<Phase>
A
A
A
B
<%>
<Ingredient>
DE-IONIZED WATER
1,3-BUTYLENE GLYCOL
MAKIMOUSSE 12
<Trade Name>
18.65
1.00
0.35
DAITOSOL 5500GM
TOTAL :
<Supplier>
DAITO KASEI
80.00
100.00
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Disperse MAKIMOUSSE 12 in 1,3-Butylene Glycol and add water to prepare gel.
2. Add phase B into Phase A and mix well.
- 13 -
3. For Peeling
Peeling Massage Lotion/Cream
No. DO-0066-AD
<Phase>
A
A
A
A
A
<Ingredient>
(CREAM BASE)
MAKILENE GC
MAKIMOUSSE 12
DE-IONIZED WATER
ALCOHOL
PRESERVATIVE
B
B
PHENYL TRIMETHICONE
DAITOSOL 5000AD
TOTAL :
Lotion
<%>
Cream
<%>
+Scrub
<%>
10.00
6.70
10.00
0.30
10.00
1.00
28.70
0.30
10.00
1.00
28.70
0.30
20.00
53.00
100.00
20.00
40.00
100.00
20.00
40.00
100.00
<Trade
d Name>
<Supplier>
l
DKE
DAITO KASEI
KF-56
Shin Etsu
DAITO KASEI
(FINAL COMPOUND)
CREAM BASE
CELLULOBEADS D-200
95.00
5.00
100.00
DAITO KASEI
<MANUFACTURING PROCEDURE>
1. Disperse MAKIMOUSSE 12 in MAKILENE GC, add the rest of Phase A, and prepare gel.
2. Prepare Phase B (Add PHENYL TRIMETHICONE to DAITOSOL 5000AD under stirring).
3 Add Ph
3.
Phase B iinto
t Ph
Phase A
A, and
dk
keep stirring
ti i until
til th
the mixture
i t
iis h
homogeneous.
4. For Lifting
Lifting Gel
No. DO-0069-SJ
<Phase>
Phase
A
A
A
A
<%>
%
5.00
0.50
0.50
84.00
<Ingredient>
MAKILENE GC
MAKIMOUSSE 12
PRESERVATIVE
DE-IONIZED WATER
B
SACRAN-05
C
C
DAITOSOL 5000SJ
DIMETHICONE (6cs)
<Trade
Trade Name
Name>
2.00
5.00
3.00
100.00
TOTAL :
<Supplier>
Supplier
DKE
DAITO KASEI
DAITO KASEI
KF-96A 6cs
DAITO KASEI
Shin Etsu
<MANUFACTURING PROCEDURE>
1. Prepare Phase A, disperse M AKIM OUSSE 12 in M AKILENE GC and preservative, and add water to prepare gel.
2. Add Phase B, and keep stirring until the mixture is homogeneous.
4. Prepare Phase C (Add DIM ETHICONE to DAITOSOL 5000SJ under stirring).
5. Add Phase C, and keep stirring until the mixture is homogeneous.
- 14 -

Similar documents

WRD Apr, 19 2016

WRD Apr, 19 2016 Never Won Four Races Three Year Olds, 116 Lbs; Older 122 Lbs Claiming Price $5 000. Five Furlongs Track Record: Magdalena May (5),121 lbs; :56 (5-19-06) Program 11 Odds Pace 11Speed

More information